NAME |
CLASSIFICATION INDEXES |
GOST 26101-84
|
FCW-Sw-19MnSiTi |
Diametr: 1,6–3,0 mm Protection: self-shielding Design: tubular, overlapping |
The Formation of the weld bead | good |
Separation of Slag | good |
Deposition Rate, kg/h | 5-10 |
Addiction Weld metal Cracking | low |
Consumption per 1 kg of wire Weld metal, kg | 1.15-1.25 |
Weld metal Hardness (HRC for 3rd-4th layer, unless otherwise stated) | after surfacing HB 260-HB 320 |
Wire diameter, mm |
Current, A |
Voltage, V |
Surfacing rate, m/h |
1,6 – 1,8 |
140 – 240 |
24 – 26 |
10 - 15 |
2,0 – 2,2 |
180 – 280 |
25 – 27 |
12 - 18 |
2,4 – 2,6 |
220 – 320 |
26 – 28 |
15 - 20 |
2,8 – 3,0 |
260 – 350 |
26 – 28 |
18 - 23 |
C | Cr | Mn | Si | Ti | S | P |
0.19 | 0.35 | 0.5 | 0.6 | 0.6 | 0.03 | 0.03 |
Brand of the wire | Distance, % | virobnik | C | Mn | Si | Cr | Ni | Cu | Mo |
ROBOFIL R 71+ (52) | 1.02 | Welding Alloys | 0.04 | 1.2 | 0.4 | ||||
ROBOFIL M 71Cu (58) | 1.05 | Welding Alloys | 0.05 | 1.1 | 0.5 | 0.5 | 0.4 | 0.4 | |
ROBOFIL KX71T1+ (53) | 1.07 | Welding Alloys | 0.05 | 1.3 | 0.5 | ||||
ROBOFIL M Mo (70) | 1.13 | Welding Alloys | 0.06 | 1.2 | 0.4 | 0.5 | |||
ROBOFIL M 71 (55) | 1.15 | Welding Alloys | 0.07 | 1.4 | 0.5 |
The diameter of the wire | 1,2–2,0 mm | 2,4–3,2 mm | 1,6–6,0 mm | |
Delivery |
Magazine B-300; S-300 |
Molded Bay | Bay | |
Standard package | cardboard box | cartons | metal drums | metal drums |
Weight, kg | 10-15 | 20-55 | 50-70 | 50-70 |