NAME |
CLASSIFICATION INDEXES |
GOST 26101-84
|
FCW-Sw-25Cr5VMoSiTi |
Diametr: 1,6–3,0 mm Protection: self-shielding Design: tubular, overlapping |
The Formation of the weld bead | good |
Separation of Slag | good |
Deposition Rate, kg/h | 5-10 |
Addiction Weld metal Cracking | moderate |
Consumption per 1 kg of wire Weld metal, kg | 1.15-1.25 |
Weld metal Hardness (HRC for 3rd-4th layer, unless otherwise stated) | after surfacing 42-51 |
Wire diameter, mm |
Current, A |
Voltage, V |
Surfacing rate, m/h |
1,6 – 1,8 |
150 – 240 |
24 – 27 |
10 - 15 |
2,0 – 2,2 |
180 – 260 |
25 – 28 |
12 - 18 |
2,4 – 2,6 |
200 – 320 |
26 – 28 |
15 - 20 |
2,8 – 3,0 |
260 – 350 |
26 – 29 |
18 - 23 |
C | Cr | Mn | Si | Mo | Ti | V | S | P |
0.25 | 5.4 | 0.8 | 1.1 | 1.1 | 0.2 | 0.45 | 0.04 | 0.04 |
Brand of the wire | Distance, % | virobnik | C | Mn | Si | Cr | Mo | W | V | Ti |
ROBODUR K 600-G (12) | 1.07 | Welding Alloys | 0.5 | 1.2 | 0.7 | 6 | 0.7 | |||
ROBODUR K 650-G (13) | 1.48 | Welding Alloys | 0.5 | 1.3 | 1.3 | 5.6 | 1.3 | 1.3 | 0.3 | |
ROBOTOOL 58-G (21) | 2.13 | Welding Alloys | 0.35 | 1.2 | 0.5 | 7 | 2.2 | 0.3 | ||
HARDFACE WLC (22) | 2.32 | Welding Alloys | 0.25 | 2 | 0.8 | 6.5 | 1.5 | 1.5 | ||
HARDFACE W (23) | 2.44 | Welding Alloys | 0.55 | 2 | 0.9 | 6.5 | 1.7 | 1.6 |
The diameter of the wire | 1,2–2,0 mm | 2,4–3,2 mm | 1,6–6,0 mm | |
Delivery |
Magazine B-300; S-300 |
Molded Bay | Bay | |
Standard package | cardboard box | cartons | metal drums | metal drums |
Weight, kg | 10-15 | 20-55 | 50-70 | 50-70 |